CLC Foam Concrete Mix Ratio: Batch Table by Density

A CLC mix is defined by three numbers, not a recipe: the target dry density, the cement content and the foam volume. For 600 kg/m³, a common starting point per cubic metre is 420 kg cement, 180 kg sand, 210 kg water and roughly 590 litres of foam. Change the density target and all four numbers move together.

Most pages on this subject either show a single lab mix or sell a foaming agent. Neither tells a site engineer what to weigh out on Monday morning when the target changes from 600 to 800 kg/m³. The tables below are planning starting points for trial batches, not certificates. Density and strength must be confirmed with your own cement, sand and foaming agent before the first structural pour.

What the ratio is actually controlling

Three properties move independently, and confusing them is the most common reason a CLC batch fails inspection.

  • Dry density is set by the mass of solids only: cement plus sand plus any filler. Foam adds almost no mass, so it controls volume, not weight.
  • Wet density is what you measure in the hopper. It runs higher than dry density because water and the water carried inside the foam bubbles are still present. A 600 kg/m³ dry mix typically places at 820–880 kg/m³ wet.
  • Strength follows density and cement content, but not linearly. Two mixes at the same dry density can differ by a full strength class if the cement-to-sand ratio differs.

That is why a ratio copied from another project often produces the right density and the wrong strength. The foam volume is transferable; the cement-to-sand split is not.

Starting batch weights per cubic metre

The table assumes ordinary Portland cement at 3.15 specific gravity, clean river or manufactured sand at 2.65, a water-to-cement ratio of 0.5, and a preformed foam at 65–75 g/L. Volumes are absolute, so they add to 1,000 litres before mixing losses.

Target dry density Cement (kg) Sand (kg) Water (kg) Foam volume (L) Indicative 28-day strength
400 kg/m³ 330 70 165 ~700 0.5–1.5 MPa
600 kg/m³ 420 180 210 ~590 1.5–3.0 MPa
800 kg/m³ 480 320 240 ~490 3.0–5.0 MPa
1000 kg/m³ 520 480 260 ~395 5.0–8.0 MPa
1200 kg/m³ 560 640 280 ~300 7.0–12.0 MPa

Strength bands are industry ranges for CLC with ordinary Portland cement and normal curing. They are not test results for a specific machine, and they shift with cement grade, sand grading, curing temperature and the accuracy of the foam generator. Read them as a screening tool, then cast cubes.

Scaling the table to your own cement and sand

When a supplier changes, or when you move from river sand to crushed sand, recalculate rather than adjust by feel. The absolute volume method takes about two minutes and prevents a whole day of rejected panels.

  1. Fix the target dry density and the cement-to-sand ratio. For 800 kg/m³ at a 60:40 split, cement is 480 kg and sand is 320 kg.
  2. Convert each solid to volume: cement 480 ÷ 3.15 = 152 L; sand 320 ÷ 2.65 = 121 L.
  3. Add water at the chosen w/c: 480 × 0.5 = 240 kg = 240 L.
  4. Sum the slurry: 152 + 121 + 240 = 513 L.
  5. Foam volume is the remainder: 1,000 − 513 = 487 L.

If your sand has a different specific gravity, only step 2 changes. If the sand is damp, weigh it wet and subtract the free moisture from the mixing water, otherwise the batch runs wet and loses density at the same foam setting.

Foam dosage and dilution

Foam is where most density error enters, because it is measured by volume and generated on site rather than delivered in bags. Typical practice is a foaming agent diluted 1:30 to 1:50 with water, expanded 20 to 25 times in a foam generator to produce foam at 60–80 g/L. Dilution and expansion ratios are specific to the agent, so confirm them with the manufacturer instead of assuming a number.

Two habits keep the dosage stable across a shift. First, set the generator once and lock the valves, then check foam density at the start and midpoint of the pour with a measuring cup. Second, never top up foam to fix a stiff mix. Add water in small increments and re-check wet density, because extra foam lowers density and strength at the same time.

When the batch misses its density

What you observe Most likely cause Correction
Wet density 80+ kg/m³ above target Foam collapsed before mixing, or too little foam charged Check foam density at the nozzle; increase foam volume in 20 L steps
Wet density below target, mix looks watery Over-mixing after foam addition, or excess water Cut mixing time after foam to 60–90 seconds; recompute w/c with damp sand
Density drifts during one pour Foam generator pressure unstable, or slurry sitting too long Fix generator pressure; place within 30–40 minutes of mixing
Density correct, cubes fail Cement-to-sand ratio too lean for the required class Hold density, raise cement and cut sand; recast trial cubes
Surface crusting, interior soft Water lost to dry substrate, or foam drainage Pre-wet substrate; reduce w/c; cover after placement

Only the first two rows are volume problems. The last three are mix design or placing problems, and adding more foam to a strength failure makes it worse.

Mixing and placing sequence

Order of addition matters as much as the ratio. Charge cement and sand dry, add about two-thirds of the water, mix to a lump-free slurry, then introduce foam and blend at low speed for 60–90 seconds. High-shear mixing after foaming destroys bubbles and raises density without any change to your weighed quantities.

Place by pump or chute, spread with a rake rather than a vibrating poker, and avoid trowelling until the surface takes a footprint without sinking. CLC is not compacted; vibration drives foam out and creates density layers that later show as cracks. For roof insulation and floor screed work, a low-output pump matched to the mix is easier to control than a high-output unit run at part load — the equipment page lists combinations for both cases at foam concrete pumping equipment.

What the ratio cannot fix

A correct ratio does not deliver structural concrete. CLC at 600 kg/m³ is insulation and void filling, not load-bearing structure, and it is not a substitute for reinforced concrete in columns or slabs. It also shrinks more than normal concrete, so joints, curing and reinforcement cover have to be designed rather than assumed.

Curing is the other limit. Foam concrete loses strength if it dries in the first three days, and in hot or windy conditions the surface can crust while the core stays plastic. Keep it covered, mist it, and do not traffic it early. Any figure for curing time or strength gain depends on density, cement content and ambient conditions — confirm it against your trial cubes rather than a generic chart.

Frequently asked questions

How much cement is in one cubic metre of CLC?

Between roughly 300 and 350 kg/m³ at the lightest practical densities and 550 to 600 kg/m³ at the heaviest, with the exact figure set by the strength class you need rather than the density alone. Below about 300 kg/m³ cement content, strength becomes unreliable whatever the density reading says.

Can I make CLC with cement and foam only, no sand?

Yes, and many roof insulation mixes do exactly that. Sand-free mixes are easier to pump and lighter, but they shrink more and cost more per cubic metre because cement fills the volume sand would occupy. Use sand where screed thickness and flatness matter.

What water-to-cement ratio should a CLC mix use?

Most site mixes run between 0.45 and 0.55. Lower than 0.45 the slurry becomes difficult to blend with foam and blocks transfer lines; higher than 0.55 the foam drains and the mix segregates. Adjust within that band to suit your mixer, not beyond it.

How soon can the surface be walked on?

Typically 24 to 48 hours for foot traffic at 600–800 kg/m³ in mild weather, longer in cold conditions or at lower densities. This is governed by strength gain, so treat the window as indicative and confirm it on site with a trial panel.

Next step

Send your target density, pour volume per shift and strength class, and we will match a mixer and pump combination to it and confirm the batch weights for the materials you actually have. Start from the foam concrete and CLC equipment range, then request the configuration sheet for your density.

Related reading

Leave a Comment

Your email address will not be published. Required fields are marked *

Scroll to Top